Problem Found: Seal Failure
One week later, we received formal feedback from the German client.
During the later stage of the thermal cycling durability test, minor air leakage occurred at the sealing lip. After disassembly, the gasket showed insufficient rebound and slight permanent deformation locally. There were no cracks, bubbles or dark spots on the surface, but the sealing contact became poor after long high-low temperature cycling. The customer suspended the mass production plan and faced risks of project delay.
German industrial customers require detailed data, root cause analysis and standardized corrective actions. They requested a failure analysis report and improvement plan within 3 working days, together with supporting material certificates.
Root Cause Analysis
We tested reserved samples in our internal lab and worked with material and molding engineers to locate the causes:
1. Material formula: The original silicone compound had weak resistance to alternating temperature aging. Its elasticity dropped quickly after thermal exposure. It met room-temperature specs but failed compression set requirements under long thermal shock.
2. Curing process: Primary curing parameters were not optimized, and post-curing time was insufficient. Low-molecular volatiles were not fully removed, hurting elastic stability at high temperature.
3. Structural weakness: The lip thickness margin was too small. Draft angle of the mold caused uneven stress when compressed, leading to stress concentration on partial areas.
Corrective Actions
1. Upgrade silicone formula: Switch to high weather-resistance fumed silica-based silicone and adjust additive system for stable compression set under extreme temperature cycles. Pre-aging tests were carried out on new material batches.
2. Optimize vulcanization process: Adjust molding temperature and holding pressure. Add standardized post-curing procedure to eliminate small molecule substances and reduce aging risks.
3. Revise mold & lip design: Strengthen thin stress-prone sections of the sealing lip, optimize runner design for uniform wall thickness and better stress distribution under compression.
4. Full inspection before delivery: New samples went through dimension audit, hardness test, compression set test and pre-conditioning air tightness test. SGS LFGB and RoHS certificates were prepared.
Re-test & Final Approval
Revised samples were sent to Germany for re-verification.
After 500 hours of thermal cycling and continuous pressure holding, no air leakage was detected. The compression set was controlled within 12%, fully passing the customer’s complete qualification test.
Cooperation Result & Client Feedback
- We solved the long-standing sealing durability issue and avoided project delay.
- This custom gasket turned into a regular repeat order. The customer also referred other German industry partners to us.
Client comment: “Your structured failure analysis, clear improvement workflow and traceable test reports meet German industrial quality standards.”
Case Takeaway
We are not only a silicone molder. We provide integrated solutions covering working condition assessment, material formulation, mold design and molding process optimization.
For EU and US industrial buyers, we support certifications including LFGB, FDA, RoHS. Custom grades available: extreme temperature resistant, ozone resistant, low compression set, conductive, flame retardant silicone rubber parts.
**Main products**: Custom profile silicone gaskets, O-rings, silicone sheets, precision compression molded silicone components
**Services**: Drawing-based custom molding, rapid prototyping, third-party testing, one-stop export service